one. Nylon fabric
1 setting temperature: 160°C—180°C, speed: 20M—25M/minute
2 The stereotyped temperature varies greatly with the color, especially the purple, pink orchid, etc., so we should pay attention to whether the color is the same after the setting and the predetermine.
3 The shrinkage rate of nylon fabric is also different.
4 Nylon fabric setting is easy to hook the yarn. If there is an end-to-end hook yarn, it should be stopped immediately. Check the nose, bellows, drum, sanding, or cloth. (such as silk stockings, mesh)
two. Polyester grey fabric shaping
1 Setting temperature: 170°C—200°C, speed: 20M—28M/minute
2 Polyester setting color generally does not change much, but the red dye sublimation fastness is not good, the chassis will leave the dye after finishing, can not do light color instantly, can only do black, can also use waste cloth more than a few times to do Light color.
3 Polyester stretch cloth fabric shrinkage rate is very large, such as customer demand for good elasticity, shrinkage, and feel good, must be scheduled to die, special attention to black and white, red and white flowers, due to dye dyeing fastness is not good, the finished product must be low temperature setting, such as High temperatures can seriously foul the product.
4 Polystyrene wave than cloth, we must pay attention to the cloth, the thickness of the edge, the temperature should be controlled well, not too high, speed slowed down, pulled in two. Two times can be set to reduce the thickness of the middle edge difference, the first time, the width is about 6-8 inches less than the finished product, g important weight of about 100 grams. The second time is 5-10 degrees lower than the first temperature, the width and weight are as required.
three. Cotton people silk
1 setting temperature 160°C-190°C, speed: 20M-30M/minute
2 If the cotton cloth is dyed directly, the cold and hot colors of the fabric will vary greatly, and the color must wait for the embryonic fabric to cool completely before the active material changes.
3 The high temperature of man wire is easy to age.
4 The cotton shrinkage rate is very high. When setting, the feeding tension should be reduced, the pressure of the pressing car should be increased, the cloth should be pressed dry, the hot air fan should be driven to the maximum, and the speed can be adjusted slowly to reduce the shrinkage rate. If the customer demand is high, It will shrink test.
5 If the customer requests that the fabric does not have a twist, it must be diagonally shaped.
IV . Silk
1 temperature 100 °C -120 °C, speed: 20M-30M / min.
2 The hot air is small and the width is fixed.
3 The silk is more delicate, you can't get water and sweat when setting it, and you can't pull it too hard.
Fives. PU adhesive
1 imported pulp, high temperature does not change color, 140 °C -180 °C, speed 25M-30M / min, large smoke.
2 domestic pulp, high temperature easy to change color, 120 °C -150 °C, speed 25M-30M, large smoke.
Fives. Weight of the door
1 Make sure to measure the weight and width before setting, if it is too far from the requirements, promptly reflect the order.
2 It is important to note that the difference between weigh and midside cannot be too far, and the difference between ç–‹ and ä¸èƒ½ cannot be too far.
3 When setting the model, please pay attention to whether it is the same before or after the cloth width.
For more content, please follow this site
When we do bulk garments, some of the buyers want to make the lining for shell fabric. We have some lining items. Both woven and knit. The lining fabric is light weight usually. We have polyester interlock and polyester chiffon for choosing. We have our color card for you to select the colors if you do not need colors that exactly match the shell fabric. And also we can do colors following your specific color. We can do a very good delivery for you if you confirm the order. If you have other special requirements on the lining fabric, please let me know. We will try to meet it.